1. Home
  2. Resources
  3. Temperature and restraint cracking
PT design guide  ·  Iron Axis engineering team

Temperature effects and restraint cracking in PT slabs

Most cracking in post-tensioned slabs is not caused by load. It comes from a slab that wants to shorten and a stiff wall, core or column that will not let it. How to estimate the movement, the restraint force, and the details that keep cracks out.

Design codes
ACI 318 · Eurocode 2 · PTI
Software
RAM Concept · AutoCAD · Revit

A post-tensioned slab shortens more than a reinforced concrete slab of the same size. The prestress squeezes it elastically, creep continues that squeeze for years, shrinkage adds its own contraction, and temperature swings move it back and forth. If the slab is free to move, none of this causes trouble. If it is tied to stiff cores, shear walls or short, stocky columns, the movement turns into tension in the slab and bending in the supports, and the slab cracks, typically near the restraining elements. In the Gulf, high ambient temperatures and large daily swings during construction make this especially relevant.

Sources of shortening

Strain contributions for a typical PT slab, each multiplied by the length from the point of zero movement (usually near the centre of stiffness of the restraining elements):

  • Elastic shortening at transfer: εel = (P/A) / Eci.
  • Creep under the sustained precompression: εcr = φ × εel, where φ is the creep coefficient for the age at loading and the exposure (see shrinkage and creep in PT slabs).
  • Shrinkage, drying plus autogenous: typically several hundred microstrain over the life of the slab in a dry, hot climate.
  • Temperature: εT = α × ΔT, with α around 10 × 10−6 per °C for normal concrete (EN 1992-1-1 §3.1.3(5)).

ΔL = Leff × (εel + εcr + εsh + αΔT)

The Gulf temperature problem

In Dubai, Abu Dhabi, Riyadh and the Eastern Province, the concrete can be cast at high temperature, then cool sharply overnight; hydration heat raises the early temperature further. Exposed roof slabs and podiums over open car parks also see large seasonal and daily swings in service. Points that matter in practice:

  • The temperature drop from the peak hydration temperature to ambient is an early restraint load, before most of the prestress is applied. Early partial stressing helps.
  • Exposed slabs (roofs, transfer levels open to the air, podium decks) need a design temperature range, often treated as a uniform change plus a gradient. The design basis should state the range used, because the governing codes require temperature effects to be included where they are significant.
  • Insulation and finishes on roof slabs reduce the service range considerably.

Indicative values. Design temperature ranges are project-specific. Use the values in the project design basis and the governing code; any figures in this guide are for illustration.

What the codes and authorities say

  • Dubai Building Code, Part F (F.6.3): elastic shortening, creep and shrinkage effects are to be taken into account where the average precompression exceeds 2.0 N/mm², a slab dimension exceeds 50 m, or there is more than one point of stiff restraint. For heavily stressed members such as transfer beams, it also asks for the effect of shortening on supporting columns and walls to be considered.
  • Ras Al Khaimah structural regulations (RAKR-S-2025): ask for temperature and lateral load effects from a 3D building model to be added to the prestress analysis.
  • ACI 318-19: §5.3.6 requires the effects of restrained volume change (shrinkage, creep and temperature) to be combined with other loads, and the commentary to §8.6.2 discusses how restraint reduces the precompression actually delivered. The PTI Post-Tensioning Manual gives guidance on pour strips and restraint.
  • TR43 and TR67 (Concrete Society): discuss restraint, joint spacing and the locations of pour strips in post-tensioned floors.

Restraint force from a column

A column fixed at both ends and pushed sideways by Δ at the slab level resists with a shear of about:

V = 12 Ec I Δ / h³    (both ends fixed)    or    V = 3 Ec I Δ / h³    (pinned at one end)

The same shear acts on the slab as a tension. Short columns at podium levels, stiff walls placed at both ends of a long slab, and cores at the extremities of the floor plate produce the largest forces. The slab tension reduces precompression and can exceed the concrete tensile strength near the restraining element, which is where cracks are usually found. For the long-term part of the movement, creep in the column relieves some of the force, so designers often use a reduced (effective) modulus.

Worked example (illustrative)

A 60 m long PT podium slab, restrained at the centre so that each end moves about 30 m. Average precompression 1.6 MPa, Eci = 24 GPa at transfer, creep coefficient 2.0, shrinkage 300 με and a temperature drop of 15 °C:

εel = 1.6 / 24 000 = 67 με    εcr = 2.0 × 67 = 133 με
εsh = 300 με    εT = 10 × 10−6 × 15 = 150 με
Total ≈ 650 με → Δ at each end ≈ 30 000 × 0.00065 ≈ 20 mm (about 39 mm over the full length)

An end column 600 × 600 mm, 4.0 m high, fixed at both ends, with an effective long-term modulus of 12 GPa (about half the short-term value, to account for creep in the column): I = 600⁴/12 = 1.08 × 1010 mm⁴, so a 20 mm movement would need V = 12 × 12 000 × 1.08 × 1010 × 20 / 4000³ ≈ 486 kN. That is a large force for one column and a large tension for the slab. The usual responses are a pour strip, a sliding or released connection at that column, or accepting cracking and providing bonded reinforcement to control it.

Indicative values. Creep, shrinkage and the effective modulus all depend on the concrete mix, humidity and age at loading. The values above are for illustration only.

Details that reduce restraint cracking

  • Pour strips (delay strips). A gap, often around 1 m wide, left between slab segments until much of the elastic and early shrinkage shortening has taken place, then cast. Tendons are stressed before the strip is cast. The strip needs propping, lapped reinforcement and sometimes couplers.
  • Locate stiff elements centrally. Cores and walls placed near the centre of the floor plate allow the slab to shorten towards them rather than tearing between two of them.
  • Temporary or permanent releases. Sliding bearings or slots at walls allow movement; temporary releases are cast up after stressing.
  • Stressing sequence. Early partial stressing controls early thermal and shrinkage cracking before full transfer.
  • Bonded reinforcement near restraints. Additional bars in the slab around walls and cores and at re-entrant corners control crack widths.
  • Movement joints in very long slabs, coordinated with the architect.

RAM Concept and similar programs can model restraint stiffness from the supports, but the long-term movement still needs a separate check. Our RAM Concept tips describe how we model the supports.

Summary

Restraint and temperature: key numbers
ItemTypical value or ruleReference
Thermal expansion coefficientAbout 10 × 10−6 per °CEN 1992-1-1 §3.1.3(5)
Elastic shortening(P/A)/EciMechanics
Creep shorteningφ × elastic strainEN 1992-1-1 §3.1.4; ACI 209
Detailed shortening check (Dubai)P/A > 2.0 N/mm², length > 50 m, or several stiff restraintsDubai Building Code Part F (F.6.3)
Column restraint shear12EIΔ/h³ (fixed-fixed)Mechanics
Pour strip widthOften about 1 m (indicative)Practice; PTI and TR43 guidance

If a slab has already cracked, our structural strengthening design and PT design review services can assess the cause and the remedy.

Part of our PT design guides. Codes are referred to by clause where we are confident of the reference, and coefficients marked indicative should be checked against the code text; always check the edition and national annex adopted for your project. Worked examples are illustrative, not designs.

S-414 FAQ

Questions we are asked about this.

Why do PT slabs crack near walls and cores?

Because the slab shortens from elastic prestress, creep, shrinkage and temperature, and stiff walls and cores resist that shortening. The resisted movement becomes tension in the slab, which is highest near the restraining elements.

What is a pour strip in a PT slab?

A temporary gap, often about 1 m wide, left between slab segments. The segments are stressed and allowed to shorten before the strip is cast, which reduces the restraint force.

How much does a PT slab shorten?

It depends on the length, precompression, creep, shrinkage and temperature. In our illustrative 60 m slab the total strain was about 650 microstrain, or roughly 39 mm over the full length.

Does the Dubai Building Code require shortening checks?

Yes. Part F of the Dubai Building Code (section F.6.3) requires elastic shortening, creep and shrinkage effects to be considered where the precompression exceeds 2.0 N/mm², a dimension exceeds 50 m, or there is more than one stiff restraint.

Does hot weather in the Gulf matter for PT slabs?

Yes. High casting temperatures and large daily swings increase early thermal shrinkage, and exposed slabs see large service temperature changes. Early partial stressing and appropriate design temperature ranges help.

Can restraint cracks be repaired?

Usually, once the cause is understood. Repairs range from crack injection to added reinforcement or releases; an assessment comes first.

S-901 Contact

Send the drawings. Get an answer from our engineers.

WhatsApp or email the architectural or structural set, the location and what you need. The reply comes from the engineers who will do the work, with a proposed scope and programme.

Office
Al Warqa 1, Dubai, UAE
Hours
Sunday – Thursday, 09:00 – 18:00 GST